Hot-Dip vs Electro-Galvanizing: Zinc Thickness, Salt Spray Hours and How to Specify

Two parts both called “galvanized” can carry ten times different coating thickness — 8 µm against 80 µm — and that one number decides whether a bin axle survives five winters at the kerb or rusts through at the weld in year two. This page covers how the two processes differ, what the standards actually require, what salt spray hours can and cannot prove, and how to write a finish callout that a plating shop cannot misread.

1. Two different processes, not two grades of one process

Electro-galvanizing (zinc plating) hangs the part as a cathode in a zinc electrolyte and builds the coating atom by atom — typically 5–25 µm, at room temperature. Nothing gets hot, so tolerances, threads and thin sheet come out exactly as they went in, with a bright, uniform cosmetic finish.

Hot-dip galvanizing immerses the part in molten zinc at roughly 445–465 °C. The zinc reacts with the steel and forms a zinc-iron alloy layer bonded to the surface, plus an outer layer of nearly pure zinc — 45–85 µm on typical fabricated steel. The bond is metallurgical, so it resists abrasion and mechanical damage far better than plating. The price is heat: thin or asymmetric weldments can distort, and stress can relieve into movement that was not there before.

A working rule: electro-zinc for appearance, tolerance and indoor parts; hot-dip for coating thickness and outdoor life. When both are needed on one assembly, the parts are finished separately and assembled afterwards — plating the assembly as a whole will always leave one surface under-protected.

2. The number to specify is coating thickness, not the word “galvanized”

On a drawing, “galvanized” alone is not a specification — it is a wish. ISO 1461 sets minimum average coating thickness for hot-dip by the thickness of the steel being coated, because thicker sections hold more heat and pick up more zinc:

Steel thicknessMin. average coating (ISO 1461)Local minimumWhat we see it on
< 1.5 mm45 µm35 µmThin brackets, covers — distort easily, usually better plated
1.5–3 mm55 µm45 µmBin body hardware, light frames
3–6 mm70 µm55 µmAxle brackets, castor forks, handle rods
≥ 6 mm85 µm70 µmStructural plates, heavy weldments

Electro-zinc is specified by class instead: ASTM B633 SC1 to SC4 corresponds to 5, 8, 12 and 25 µm, with ISO 2081 expressing the same idea in micrometres directly, plus a finish type for the passivation (clear/blue, yellow, black). If the drawing says only “zinc plated”, most shops will default to the cheapest class that passes a visual check — which is how 5 µm ends up on an outdoor part.

3. What salt spray hours can and cannot tell you

Neutral salt spray (ASTM B117 / ISO 9227: 5% NaCl fog, 35 °C, continuous) is the test every buyer quotes and almost nobody interprets correctly. Two events are reported separately: white rust, when the zinc itself starts to corrode, and red rust, when the base steel is reached. Only the second one means the part has begun to fail.

FinishTypical thicknessIndicative NSS to red rustRealistic service
Electro-zinc, clear/blue5–12 µm48–96 hIndoor, dry, handled parts
Electro-zinc, yellow8–15 µm72–120 hHumid indoor, sheltered outdoor
Hot-dip galvanized45–85 µm200–500 hOutdoor, kerbside, structural
E-coat over zinc15–25 µm240–400 hComplex shapes, sharp edges
Powder coat, pretreated60–90 µm300–500 hVisible parts, colour matching

What the test cannot do is predict service life by multiplication. A 500-hour coupon and a twenty-year bin axle are not related by a formula: real exposure adds wet–dry cycling, chloride deposition, UV, grit abrasion and mechanical knocks, and it attacks exactly the places a flat coupon does not have — sheared edges, weld seams, thread crests, the inside of a closed tube. Hot-dip wins on edges because the alloy layer wraps them; electro-zinc is thinnest precisely where the current density was lowest. Trivalent passivation films also lift early salt spray hours without changing three-year performance, which is why two suppliers can quote 96 h and 240 h for what is effectively the same coating.

Our position: treat salt spray as a batch-consistency check, not a warranty. We run coupons with each coating batch, supply third-party (SGS) neutral salt spray reports on request, and say plainly when a salt spray figure does not apply to your geometry.

4. Match the coating to the environment, not to the catalogue

ISO 9223 groups service environments by corrosivity and gives a first-year zinc loss for each. Divide the coating thickness by that rate and you get an order-of-magnitude life — then discount it, because edges, drainage and handling decide the rest:

CategoryTypical environmentZinc loss, 1st yearOur usual finish
C2Indoor, rural, dry stores< 0.7 µmElectro-zinc 8–12 µm
C3Urban, light industrial, inland city kerbside0.7–2 µmHot-dip 55–70 µm, or e-coat 20 µm
C4Coastal, heavy industrial, de-icing salt2–4 µmHot-dip 70–85 µm
C5Marine splash, chemical plant4–8 µmHot-dip 85 µm + topcoat, or zinc-nickel + e-coat

A 70 µm hot-dip coating in C3 works out at a theoretical 35-plus years, but we quote 15–25 years for kerbside bin hardware and 8–12 years on a coastal C4 site, because edges, hinges and impact damage write the real service life. The same arithmetic on 8 µm of electro-zinc in C4 gives two to four years — which is exactly why plated bin axles are rusting at the weld while the rest of the part still looks new.

5. Design rules that decide whether hot-dip works at all

6. How to write the finish callout

Weak calloutWhat it usually producesCallout that works
“Galvanized”Whatever class the shop ran that week“Hot-dip galvanized to ISO 1461; average coating ≥ 70 µm on 4 mm steel; M8 threads tapped after galvanizing”
“Zinc plated”5 µm clear, no bake“Electro-zinc to ASTM B633 SC3 Type II (12 µm min), trivalent clear passivation, bake 4 h at 200 °C within 4 h of plating”
“Rust proof”Oil film, gone by arrival“C4 coastal service; propose finish and state expected salt spray hours”

Two more lines are worth adding to any drawing: which surfaces must stay coating-free (bearing bores, ground diameters, thread fits), and whether touch-up of damaged areas is permitted — and with what. Both are questions a plating shop will otherwise answer for you.

7. What should ship with the order

Coating thickness measured with a calibrated gauge on every batch, with the readings attached to the packing list; a third-party salt spray report when the finish is carrying a corrosion promise; material certificates for the steel; and photos of the finished parts before packing. Ask for these in the RFQ — after the container has sailed, no report can be recreated. Full process ranges, tolerances and the finish table sit on our metal fabrication page; the parts where corrosion most often decides the argument are waste bin axles and wheels and industrial casters.